Lap splice length is the number most rebar crews and estimators ask for, and the code does not give a single one. ACI 318 gives a rule: the splice length is a multiple of the bar's development length, which depends on bar size, concrete strength, steel grade and a few modification factors. This guide explains that rule in plain terms, gives a lap splice length chart for common conditions, and works an example. Lengths are in inches, with millimeters where useful.
Development length and lap splice: what is the difference?
Development length, written ℓd, is how far a bar must be embedded in concrete before it can carry its full yield stress. A lap splice joins two bars by overlapping them, and the stress passes from one bar to the concrete and back into the other. For that reason ACI 318-19, Section 25.5.2.1, sets the tension lap splice length ℓst from ℓd, using the factors in Table 25.5.2.1.
The ACI 318-19 development length formula
ACI 318-19, Table 25.4.2.3, gives the tension development length of deformed bars. The table has two rows of conditions and two bar groups. In each case ℓd is also never less than 12 in. (Section 25.4.2.1).
| Conditions | #6 and smaller | #7 and larger |
|---|---|---|
| Clear spacing of bars at least 2db and clear cover at least db (or spacing at least db with cover at least db and ties or stirrups throughout) | ℓd = (fy ψt ψe ψg ÷ 25λ√f'c) db | ℓd = (fy ψt ψe ψg ÷ 20λ√f'c) db |
| Other cases | ℓd = (3 fy ψt ψe ψg ÷ 50λ√f'c) db | ℓd = (3 fy ψt ψe ψg ÷ 40λ√f'c) db |
Here fy is the yield strength in psi, f'c is the specified concrete strength in psi, and db is the bar diameter. The modification factors come from ACI 318-19, Table 25.4.2.5:
| Factor | Condition | Value |
|---|---|---|
| ψt (casting position) | More than 12 in. of fresh concrete below the bar (top bars) | 1.3 |
| ψt | Other | 1.0 |
| ψe (coating) | Epoxy-coated, cover less than 3db or spacing less than 6db | 1.5 |
| ψe | Epoxy-coated, all other conditions | 1.2 |
| ψe | Uncoated or galvanized | 1.0 |
| ψg (grade) | Grade 40 or 60 / Grade 80 / Grade 100 | 1.0 / 1.15 / 1.3 |
| λ (concrete weight) | Normalweight / lightweight | 1.0 / 0.75 |
The product ψtψe need not exceed 1.7. The code also limits the √f'c used in the equation, so very high strengths do not shorten the length any further. For what f'c means and how it is tested, see our guide to concrete compressive strength.
Lap splice classes: Class A and Class B
ACI 318-19, Table 25.5.2.1, sets the tension lap splice length by the amount of steel provided and the share of bars spliced at one location.
| As provided / As required | Max % of As spliced in the lap length | Splice class | Lap length ℓst |
|---|---|---|---|
| 2.0 or more | 50% | Class A | 1.0 ℓd, at least 12 in. |
| 2.0 or more | 100% | Class B | 1.3 ℓd, at least 12 in. |
| Less than 2.0 | All cases | Class B | 1.3 ℓd, at least 12 in. |
In practice, most splices are Class B, because splicing at points where the provided steel is at least double the required steel is the exception. Splice locations should be chosen by the engineer of record.
Rebar lap splice length chart (Grade 60, 4,000 psi)
The chart and table below apply the simple Table 25.4.2.3 equations for one common case: Grade 60 bars (ψg = 1.0), 4,000 psi normalweight concrete (λ = 1.0), uncoated bars (ψe = 1.0), bottom bars (ψt = 1.0), and clear spacing at least 2db with clear cover at least db. Bar diameters are from ASTM A615 (see our rebar size chart). Values are rounded up to the next inch. The millimeter column converts those rounded-up inch values at 25.4 mm per inch and rounds to the nearest millimeter, so both columns are on the same basis. These are worked examples for the stated conditions, not field cut lengths.

| Bar | db (in.) | ℓd (in.) | Class A lap (in.) | Class B lap (in.) | Class B lap, other cases (in.) | Class B lap (mm, from rounded in.) |
|---|---|---|---|---|---|---|
| #4 | 0.500 | 19 | 19 | 25 | 37 | 635 |
| #5 | 0.625 | 24 | 24 | 31 | 47 | 787 |
| #6 | 0.750 | 29 | 29 | 37 | 56 | 940 |
| #7 | 0.875 | 42 | 42 | 54 | 81 | 1372 |
| #8 | 1.000 | 48 | 48 | 62 | 93 | 1575 |
| #9 | 1.128 | 54 | 54 | 70 | 105 | 1778 |
| #10 | 1.270 | 61 | 61 | 79 | 118 | 2007 |
| #11 | 1.410 | 67 | 67 | 87 | 131 | 2210 |
Check: for the #8 bar, ℓd = 60,000 ÷ (20 × √4,000) × 1.0 in. = 47.4 in., so Class B = 1.3 × 47.4 = 61.7 in., rounded up to 62 in. The ACI commentary gives the same 47 db figure for this case.
Change any condition and the numbers change. Top bars, epoxy coating, lightweight concrete, Grade 80 steel or tight spacing all make the lap longer. Higher f'c shortens it. Always confirm against the project drawings.
Worked example: #6 top bars, Class B
A designer specifies #6 top bars (Grade 60, 4,000 psi, uncoated, normalweight), with more than 12 in. of concrete below the bars, clear spacing of 2db and cover of db. The splice is Class B.
- db = 0.750 in. (#6)
- ℓd = 60,000 × 1.3 (ψt) × 1.0 × 1.0 ÷ (25 × 1.0 × √4,000) × 0.750 in. = 37.0 in.
- ℓst (Class B) = 1.3 × 37.0 = 48.1 in., round up to 49 in.
The same bar as a bottom bar needs 37 in. The top bar penalty is the 30 percent from ψt. See also how bars are counted in our construction takeoff guide, and how mix strength affects the numbers in our concrete mix design basics.

Common mistakes
- Using one number for every bar size. Lap length grows with bar diameter.
- Assuming Class A for splices that need Class B.
- Forgetting the 30 percent increase for top bars.
- Ignoring spacing and cover, which move the bar into the "other cases" row.
- Applying US values on a project under a different code. This guide covers ACI 318-19 only. Projects under SBC or ECP use their own tables.
Frequently asked questions
What is the lap splice length for #4 rebar?
For a #4 bar (Grade 60, 4,000 psi concrete, uncoated, bottom bar, clear spacing at least 2 bar diameters, cover at least 1 bar diameter), the development length under ACI 318-19 Table 25.4.2.3 is about 19 in. A Class B tension lap is 1.3 times that, about 25 in. Your drawings and local code govern.
What is a Class B splice?
In ACI 318-19 Table 25.5.2.1, a Class B tension lap splice is 1.3 times the development length, and no less than 12 in. It is required whenever the provided steel is less than twice the required steel, and it is also used when more than 50 percent of the bars are spliced at one location.
What is the difference between development length and lap splice length?
Development length is the embedment a bar needs to transfer its full stress into the concrete. A lap splice length is the overlap of two bars, set as a multiple of the development length (1.0 for Class A, 1.3 for Class B), with a minimum of 12 in.
Does the lap length change for top bars?
Yes. ACI 318-19 Table 25.4.2.5 gives a casting position factor of 1.3 for horizontal bars with more than 12 in. of fresh concrete placed below them. That increases development length and the lap by 30 percent, subject to the product limit of 1.7 with the epoxy factor.
Can I use this chart on a real project?
Use it for estimating and checking. The numbers assume one common set of conditions. The structural drawings, the engineer of record and the locally adopted code govern the lap lengths you build.
Sources
- American Concrete Institute, ACI CODE-318-19, Building Code Requirements for Structural Concrete: Section 25.4.2.1 and Tables 25.4.2.3 and 25.4.2.5 (tension development length), Section 25.5.2.1 and Table 25.5.2.1 (tension lap splice length). Clause numbers only; consult the code for full text.
- ASTM A615/A615M, Standard Specification for Deformed and Plain Carbon-Steel Bars for Concrete Reinforcement (bar diameters), as used in our rebar size chart: https://www.handasa.xyz/2026/11/rebar-size-chart-astm-a615-weights.html
Read also: Concrete Cover for Rebar: ACI 318-19 Minimum Cover by Exposure